Tensile and Flexural Testing of Rigid Plastics

Why Tensile and Flexural Testing Matters for Plastics

Tensile and flexural tests rank among the mechanical tests most often applied to plastics. A tensile test pulls a specimen along its axis while the laboratory logs how much it elongates; a flexural test bends a bar and logs how far it deflects. Both generate stress-strain data from which strength and stiffness are derived, and both are typically carried out on a universal testing machine. ISO 527-1 lays down the general principles for determining the tensile properties of plastics and plastic composites [1], while ISO 178 addresses the flexural properties of rigid and semirigid plastics [3]. ASTM International offers counterpart methods: ASTM D638 for tensile properties [5] and ASTM D790 for flexural properties [7].

The value of a result depends on the conditions under which it was produced. ASTM D638 notes that tensile properties shift with the way specimens are prepared and with the testing speed and environment, so these must be tightly controlled whenever precise comparisons are needed [5]. A laboratory consequently requires more than a machine: it needs a documented path from raw material to specimen, a fixed conditioning routine, a verified instrument and consistent recording of test conditions.

This article walks through how tensile and flexural testing of rigid plastics is done, what the principal standards demand, the usual points at which results go astray, and the factors to weigh when picking a universal testing machine. It is aimed at polymer engineers, quality control personnel, laboratory technicians and purchasing managers. It reflects general practice and published requirements; it is no substitute for the full text of whichever standard governs your test, and it gives no operating instructions for any specific machine.

Note on standard editions. Standards are updated periodically, so verify the current edition before drafting a test procedure. The editions identified as current when this was written were ISO 527-1:2019 [1], ISO 527-2:2025 [2], ISO 178:2019 [3], ASTM D638-22 [5] and ASTM D790-25 [7]. One standards catalogue shows ISO 527-1:2019 and ISO 178:2019 as scheduled for revision, with new versions under development [1][3]. Certain ASTM D790 figures cited below are taken from the 2017 edition and are marked where they occur.

What Tensile and Flexural Tests Determine

Tensile properties

ISO 527-1 specifies methods for determining tensile strength, tensile modulus and other aspects of tensile stress-strain behaviour [1]. The 2019 edition applies to rigid and semirigid thermoplastics and thermosets, among them filled and reinforced compounds, sheets, laminates and fibre reinforced composites; rigid cellular materials are normally outside its scope and are handled under ISO 1926 [1]. ISO 527-2 then supplies the test conditions for moulding and extrusion plastics [2]. ASTM D638 covers unreinforced and reinforced plastics tested as dumbbell specimens up to 14 mm thick, and sends thin sheeting under 1.0 mm to ASTM D882 [6].

Flexural properties

ISO 178 determines flexural strength, flexural modulus and other aspects of flexural stress-strain behaviour, using a freely supported beam loaded at its midpoint, an arrangement called three point loading [3]. ASTM D790 likewise applies three point loading to a simply supported beam and is generally suited to rigid and semirigid materials [8]. In three point bending, stress and strain peak on the specimen's underside, directly beneath the loading point [19].

What the results can and cannot be used for

ASTM D638 presents its data as appropriate for controlling and specifying plastic materials, for qualitative characterisation, and for research and development [6]. ASTM D790 observes that flexural properties are particularly valuable for quality control and specification [7]. ISO 178 says its method does not yield design parameters, although it can be used for materials testing and as a quality control test [4]. ASTM D638 adds a warning: because many plastics respond to strain rate and environment, results should not be assumed valid for applications whose loading rates, durations or surroundings differ greatly from those of the test [6].

StandardProperty testedScope points relevant to rigid plastics
ISO 527-1:2019Tensile (general principles)Covers rigid and semirigid thermoplastics and thermosets, such as filled and reinforced compounds, sheets, laminates and fibre reinforced composites. Rigid cellular materials are normally excluded [1]
ISO 527-2:2025Tensile (test conditions)Sets test conditions for moulding and extrusion plastics, building on ISO 527-1. Flexible films and sheets under 1 mm thick are outside its scope and belong to ISO 527-3 [2]
ISO 178:2019Flexural (three point)Applies to rigid and semirigid plastics, using a freely supported beam loaded at midspan [3]
ASTM D638-22TensileUnreinforced and reinforced plastics tested as dumbbell specimens up to 14 mm thick. Thin sheeting below 1.0 mm is referred to D882 [6]
ASTM D790-25Flexural (three point)Rigid and semirigid materials. No flexural strength can be reported when the specimen neither breaks nor yields before reaching the 5.0 % strain limit [8]

Table 1. Core standards covering tensile and flexural testing of rigid plastics

The standards are not interchangeable. ASTM D790 itself points out that it and ISO 178 address the same subject but differ in technical content [9].

Tensile Testing of Rigid Plastics: ISO 527 and ASTM D638

Principle

In a tensile test, both ends of the specimen are clamped and it is extended at a controlled rate while force and extension are logged. ASTM D638 calls for recording the load-extension curve together with the load and extension at yield (where yield occurs) and at rupture [6]. Tensile strength is the peak load divided by the mean original cross-sectional area within the gauge length [6]. Where the material has an initial linear region, the modulus is calculated from it; where no proportional region is apparent, ASTM D638 applies a secant modulus at a designated strain [6]. Figure 1 illustrates these features schematically.

Schematic stress-strain curves for a rigid plastic. Curve A yields and then draws before breaking, whereas curve B fractures without yielding. The curves are for illustration only and are not measured data for any material.
Figure 1: Schematic stress-strain curves for a rigid plastic. Curve A yields and then draws before breaking, whereas curve B fractures without yielding. The curves are for illustration only and are not measured data for any material.

ASTM D638 also remarks that the term elastic modulus is contested for plastics, and the value is best interpreted as a measure of stiffness under the stated test conditions [6].

Tensile specimens

Tensile specimens for rigid plastics are dumbbell shaped: wide grip ends, a narrower parallel section and a marked gauge length (Figure 2). ISO 527-2 permits specimens moulded directly to the chosen dimensions as well as ones machined, cut or punched from injection or compression moulded plates. Its 2012 edition designated the multipurpose specimen as preferred and pointed to ISO 20753 [24]. ISO 527 employs type 1A and type 1B dumbbells. A manufacturer application note gives both a parallel section 4 mm thick and 10 mm wide, with gauge lengths of 75 mm for type 1A and 50 mm for type 1B [18]. Verify every dimension against the current standard, since the 2012 text referenced here predates ISO 527-2:2025.

Schematic of a dumbbell tensile specimen, labelling the grip sections, transitions, parallel section, gauge length and width b. Not drawn to scale; dimensions are given in the relevant standard.
Figure 2: Schematic of a dumbbell tensile specimen, labelling the grip sections, transitions, parallel section, gauge length and width b. Not drawn to scale; dimensions are given in the relevant standard.

Comparable test data depends on standard specimens, and ISO 20753 supplies their designations and dimensions. The 2023 edition names type A (tensile, multipurpose or reduced scale), type B (bar), type C (small tensile), type D (square plate) and type F (rectangular plate) [10], and it has replaced the withdrawn 2018 edition [22].

ASTM D638 follows a different scheme, offering specimen Types I to V selected according to the rigidity and thickness of the material. Type I is preferred for material up to 7 mm thick, and Type II is recommended if a material fails to break in the narrow section of a Type I specimen. Type V is for cases where only material 4 mm thick or less is available, while Type III is mandatory for thicknesses above 7 mm up to 14 mm [6]. Specimens may be injection moulded, machined or die cut [6].

Test speed and strain measurement

The governing standard or material specification fixes the test speed. ASTM D638 (Table 1) gives 5, 50 and 500 mm/min for Types I to III and 1, 10 and 100 mm/min for Type V; consult it for the speed designation that matches your material. If none is specified, the slowest speed that ruptures the specimen within 0.5 to 5 minutes applies [6]. One testing laboratory, describing ISO 527 practice, says 5 or 50 mm/min is typical for strength and elongation and 1 mm/min for modulus [17].

Modulus is the hardest quantity to get right in a tensile test. A machine manufacturer observes that ISO 527 evaluates strain between 0.05 % and 0.25 %, so strain measurement must be very precise [16]. For modulus, ASTM D638 demands an extensometer of Class B-2 or better and forbids deriving modulus or elongation from crosshead or grip separation [6]. It also requires toe compensation, except where the toe region reflects genuine material behaviour [6].

Flexural Testing of Rigid Plastics: ISO 178 and ASTM D790

Principle and geometry

In ASTM D790, a rectangular specimen sits on two supports while a loading nose presses on it midway between them [9]. The specimen has to be solid and uniformly rectangular, with a depth no greater than its width [9]. Figure 3 sketches the geometry.

Schematic three point flexural test geometry. A rectangular bar lies on two supports and is loaded by a central nose. The key dimensions are the support span L and the specimen depth h. Not to scale.
Figure 3: Schematic three point flexural test geometry. A rectangular bar lies on two supports and is loaded by a central nose. The key dimensions are the support span L and the specimen depth h. Not to scale.

ISO 178 specimen and test speed

ISO 178 prefers a specimen of 80 mm × 10 mm × 4 mm and tolerates other widths where that size is unattainable [15]. Machining from sheet (ISO 2818), compression moulding (ISO 293 and ISO 295) and injection moulding (ISO 294-1 and ISO 10724-1) are all accepted routes [15]. There are two test methods. Method A holds the strain rate at 1 %/min from start to finish; Method B measures modulus at 1 %/min and then moves to 5 %/min or 50 %/min, chosen by the ductility of the material, for the rest of the curve [19]. As these rates come from a property reference page, check them in the standard before writing a procedure. Support span is linked to specimen thickness, and the ratio required should be read from the standard.

ASTM D790 specimen, procedures and strain limit

ASTM D790 names a preferred specimen of 127 mm × 12.7 mm × 3.2 mm for moulding materials, tested at a span to depth ratio of 16 to 1, while sheet of 1.6 mm or more is tested at a span of 16 ± 1 times its depth [9]. If the tensile to shear strength ratio of a laminate or high strength composite is high, larger ratios may be needed [9]. This paragraph and the next draw on the 2017 edition of D790 [9]; because the current edition is D790-25 [7], check the values against it.

ASTM D790 provides two procedures. Procedure A, at a strain rate of 0.01 mm/mm/min, is preferred for materials that fail at small deflections; Procedure B, at 0.10 mm/mm/min, is for materials that neither break nor yield within 5.0 % strain under Procedure A conditions [9]. A test ends at 5.0 % outer fibre strain or on fracture, whichever comes first [9]. It follows that flexural strength cannot be determined for a material that neither breaks nor yields within that limit [8], and ASTM proposes four point bending as a better fit for materials that have not ruptured by the maximum strain allowed [8]. Figure 4 shows the three cases schematically.

Schematic flexural stress-strain curves drawn against the 5.0 % strain limit of ASTM D790. Curve A fractures first, curve B yields first, and curve C arrives at the limit with neither fracture nor yield, leaving no flexural strength to report under this method. Illustrative only.
Figure 4: Schematic flexural stress-strain curves drawn against the 5.0 % strain limit of ASTM D790. Curve A fractures first, curve B yields first, and curve C arrives at the limit with neither fracture nor yield, leaving no flexural strength to report under this method. Illustrative only.

Comparing ISO 178 and ASTM D790

ISO 178 and ASTM D790 part ways on several practical points. Their preferred specimen depths are 4 mm and 3.2 mm respectively, and since test speed is tied to depth, the speeds they call for can differ. ASTM D790 allows one test speed throughout, while ISO 178 permits a second, faster speed after modulus has been determined [15]. Any result should therefore be reported together with the method that produced it.

ItemTensile testThree point flexural test
LoadingAxial pulling of a dumbbell shaped specimen [6]A rectangular bar bent under a load at midspan [8]
Main outputsTensile strength, tensile modulus and associated strain values [1]Flexural strength, flexural modulus and the flexural stress-strain curve [3]
Typical limitationOutcome is affected by specimen preparation, speed and environment [5]Flexural strength is unavailable when the specimen neither breaks nor yields within 5.0 % strain (ASTM D790) [8]
Stated useControlling and specifying materials, characterisation, and research and development [6]Particularly valuable for quality control and specification [7]

Table 2. Comparison of tensile and flexural tests

Specimen Preparation

Specimen preparation lies between the raw material and the test and is a leading cause of disagreement between laboratories, because tensile properties are known to change with how specimens are made [5]. The routes below are those named in the standards and sources reviewed.

Routes to a specimen

  • Moulded directly to size. ISO 527-2 permits specimens moulded to the chosen dimensions [24]. ISO 178 specimens can be injection or compression moulded following the ISO moulding standards [15], and ASTM D638 includes injection moulding among its routes [6].
  • Machined or cut from sheets. ISO 178 specimens can be machined from sheets [15]. ASTM D638 also lists machining and die cutting [6], and ASTM D790 allows machining as long as it is reported [9].
  • Compression moulded plates. Under ISO 527-2, specimens may be machined, cut or punched from injection or compression moulded plates [24].

Surface quality and dimensions

Surfaces on an ASTM D638 specimen must be free of flaws and flash, and gauge marks may not be scratched or punched into it [6]. ASTM D790 sets a flatness and parallelism limit of ±0.2 mm for opposite faces [9]. Both standards also require width and thickness to be measured before testing. D638 asks for the nearest 0.025 mm, taken at the centre and within 5 mm of either end of the gauge length [6]; D790 asks for 0.03 mm, tightening to 0.003 mm where depth is under 2.54 mm [9].

Orientation and anisotropy

Processing by moulding or extrusion may leave chains, fillers and fibres partly lined up in one direction. For this reason ASTM D638 warns that orientation from moulding can change properties, and requests two sets of specimens, one cut parallel to the suspected direction of anisotropy and one normal to it [6]. For anisotropic sheet, ASTM D790 wants five specimens or more in each direction stated [9]. ISO 178 points out one more factor: in injection moulded semicrystalline polymers especially, the oriented skin layer varies in thickness with moulding conditions and this too affects flexural behaviour [3]. Research bears this out, since flow induced alignment of rubber particles in injection moulded mass polymerised ABS made it stiffer in tension along the flow [20].

Conditioning and Test Environment

ASTM D618 sets out how plastics are conditioned for testing, not necessarily to equilibrium, and the conditions for testing them [14]. Its standard laboratory atmosphere is 23 °C at 50 % relative humidity, within stated tolerances [14]. Unless told otherwise, ASTM D638 and ASTM D790 both specify conditioning to Procedure A of D618 and testing at the temperature and humidity used for conditioning [6][9]. ISO 291 likewise provides standard atmospheres for conditioning and testing plastics, including 23 °C and 50 % relative humidity [13]. Since ASTM D618 concedes that it differs technically from ISO 291 [14], the atmosphere should come from the governing standard or specification.

Test temperature is important as well. One testing laboratory reports that tensile tests can be run at ambient, elevated or reduced temperatures, with a thermal chamber enclosing the specimen and grips [17].

Universal Testing Machines for Tensile and Flexural Testing

Most tensile and flexural testing of plastics takes place on a universal testing machine (UTM) driven at a constant rate of traverse. ISO 5893:2019 lays out what such tensile testing systems for rubbers, plastics and adhesives must meet, and extends to their use in flexural, shear and compression work [11]. The headings in its contents page run through machine class, size and construction, axial alignment, grips, drive characteristics, force measuring systems, steady state and dynamic accuracy, elongation or deflection measurement, rate of displacement, machine stiffness, stability and the certificate of verification [21].

Force measurement and verification

ISO 7500-1:2018 concerns the calibration and verification of tension and compression testing machines, covering a general inspection, calibration of the force measuring system and a check that performance stays inside the limits of a given class [12]. Because it concerns static calibration, its values may not apply to high speed or dynamic testing [12]. According to manufacturer application notes, ISO 527 demands force accuracy equal to ISO 7500-1 Class 1 (within 1 % of the indicated force) and ASTM D790 demands accuracy meeting ASTM E4 Class 1 [18][23]. The precise accuracy requirement should be confirmed in whichever standard you apply.

Grips, fixtures and strain devices

  • Tensile grips. ASTM D638 requires the specimen to be aligned with the grips and clamped firmly enough to stop slippage without crushing it [6].
  • Extensometer. A suitable extensometer is required to obtain tensile modulus, as described above [6]. Take the required class and accuracy from the governing standard.
  • Flexure fixture. The nose and the supports are set by ASTM D790 to a standard radius of 5.0 ± 0.1 mm; a different radius is acceptable if it is specified or agreed and then reported. Span setting must land within 1 % of the required figure [9].
  • Deflection measurement. ASTM D790 lets deflection be taken from crosshead position or a deflectometer, and the chosen method must be reported [8]. Correcting for machine compliance is optional [9].

The Test Procedure in Outline

Figure 5 charts a generic workflow that suits both tests. It does not replace the operating procedure of any particular machine, and the governing standard and machine manual always take precedence.

Generic workflow for tensile and flexural testing of rigid plastics, from choosing the standard through to reporting. Anything specific to a machine is taken from its manual.
Figure 5: Generic workflow for tensile and flexural testing of rigid plastics, from choosing the standard through to reporting. Anything specific to a machine is taken from its manual.
  1. Select the method. Pick the standard and specimen type demanded by the material specification or agreed with the customer. ASTM D638 states that when a material specification modifies a method, the modification takes precedence [6].

  2. Prepare and inspect specimens. Look for flaws, flash and surface damage [6].

  3. Condition. Apply the atmosphere given in the standard or specification [6][9][13].

  4. Measure width and thickness. Use the positions and resolution the standard gives [6][9].

  5. Mount the specimen. For tensile work, seat the specimen square in the grips; for flexure, centre it across the supports. Then attach whichever strain or deflection device the method uses [6][9].

  6. Run the test. Run at the speed the method prescribes, switching to a separate modulus speed where the standard calls for one [6][15].

  7. Evaluate and report. Reporting under ASTM D790 must cover the procedure used, how deflection was measured, the support span, the specimen dimensions and any non-standard radii. The mean is quoted to three significant figures and the standard deviation to two [9].

Both ASTM methods insist on five or more specimens per sample for isotropic materials [6][9]. A specimen that breaks at an obvious flaw, or in the tensile case beyond the narrow section, is rejected and replaced, unless the flaw happens to be what is being investigated [6][9].

Causes of Variability and Common Pitfalls in Plastics Testing

Because plastics respond strongly to how they are processed and tested, most scatter in tensile and flexural data traces back to a short list of causes. Table 3 lists them along with the controls described in the cited sources. Tables 1 and 2 earlier in the article summarise the standards themselves.

FactorWhy it mattersControl described in sources
Specimen preparation and orientationTensile properties change with specimen preparation, and moulding orientation can alter them [5][6]Prepare compared samples by the same route. Test both parallel and normal to a suspected orientation [6]
Test speedProperties depend on speed [5], and flexural properties depend on strain rate [9]Apply the speed the standard or specification requires [6][9]
Environment and conditioningPlastics are affected by humidity and temperature [14]Condition and test in one and the same atmosphere [6][9][14]
Specimen dimensionsFlexural properties depend on specimen depth [9]Measure every specimen as specified and hold the span within 1 % of target [9]
Strain measurementCrosshead displacement is not allowed for tensile modulus [6]Fit an extensometer of the required class [6] and state how flexural deflection was measured [8]
Flaws and failure locationFractures at flaws or outside the narrow section produce unrepresentative values [6]Discard and retest, unless the flaw is itself under study [6][9]
Machine conditionThe accuracy of the force reading influences the result [12]Calibrate and verify the force system [12]. ISO 5893 sets out machine requirements [11]

Table 3. Main causes of variability in tensile and flexural testing

Frequent practical issues

  • Grip slippage or crushing. Clamp firmly enough to prevent slippage but not so hard that the specimen is crushed [6].
  • Failure outside the gauge section. A tensile specimen that fractures at a flaw, or outside the narrow section, is rejected and a replacement is tested [6]. Do not confuse this with choosing a specimen type: for a material that will not break in the narrow section of a Type I specimen, ASTM D638 recommends changing to Type II [6].
  • Toe region at the start of the curve. A slow, curved start to the trace often reflects slack being pulled out of the system rather than the material itself. Both ASTM D638 and ASTM D790 deal with this through toe compensation, described in Annex A1 [6][9].
  • No break or yield in a flexural test. Flexural strength cannot be assigned when neither event occurs within the 5.0 % limit (Figure 4). For such materials ASTM D790 points to Procedure B or four point bending [8][9].

Choosing a Universal Testing Machine for Plastics

Start from the test itself, not from a brochure. Write down the standards you are bound to, the specimens you will run and the results you must report; only then compare a machine's published specifications to that list. Table 4 draws its criteria from the standards and sources cited in this article.

CriterionWhat to checkBasis
Standards and specimensThe tensile and flexural methods you must run, with their specimen types and sizes[1][3][6][8]
Force range and classCapacity adequate for your strongest specimens, plus the force measurement class the method demands[11][12][18]
Speed rangeThe speeds your chosen standards require. Table 1 of ASTM D638 ranges from 1 to 500 mm/min[6]
Strain and deflection measurementAn extensometer for modulus, and a deflectometer or crosshead option for flexure[6][8]
Grips and fixturesGrips that fit your specimens, and a flexure fixture offering the required span and nose radii[6][9]
Temperature capabilityA thermal chamber if testing is needed away from ambient temperature[17]
Verification and documentationCalibration and verification certificates, and the machine class[11][12]
Data handlingData acquisition sufficient for the curve features you evaluate[18]
Space, utilities and safetyBench or floor space, power supply and guarding as set out in the manualMachine manual

Table 4. Checklist for selecting a machine for tensile and flexural testing of rigid plastics

A machine is just one element of a compliant test; fixtures, strain devices, specimens and conditioning count equally. Whatever is sold as a universal testing machine should be checked against every method you intend to run.

Maintenance, Safety and Good Laboratory Practice

Maintenance, lubrication, guarding and emergency procedures belong to the manufacturer's manual. Because intervals and safety ratings vary from machine to machine, none are given here. The standards themselves pass safety to the user: ASTM D790 disclaims any attempt to cover every safety concern and makes the user responsible for establishing safety and health practices [8], and ISO 7500-1 cautions that a few of its specified tests involve processes with the potential to create a hazard [12].

  • Verify the force measuring system as the method and your quality system require [12].
  • Record the standard and edition, specimen type, preparation route, conditioning, test speed, strain or deflection measurement method, grips or fixture, and any deviations [9].
  • Keep preparation and conditioning identical for samples you plan to compare [6][9].
  • Whenever a specimen is thrown out and retested, write down why [6][9].

Frequently Asked Questions

Can ISO and ASTM results be compared directly?

Not safely. Per ASTM D790, it and ISO 178 treat the same subject yet differ technically [9]; their preferred specimen depths and test-speed schemes also differ [15]. Always quote the method and edition alongside a result.

Should I run a tensile test or a flexural test?

The two tests address different needs. One stretches a dumbbell shaped specimen in uniaxial tension; the other bends a rectangular bar over three points (Table 2). Let the material specification or the customer's requirement decide, because each method describes the uses it is meant for [6][7].

How many specimens should be tested?

Where the material is isotropic, five or more specimens per sample are required by both ASTM D638 and ASTM D790 [6][9]. Under any other standard, the specimen count is found in its own text.

Can these results be used directly for design?

ISO 178 states that its method is unsuitable for determining design parameters but can be used for materials testing and quality control [4]. ASTM D638 warns that its data may not apply where load and time scales or environments differ widely from those of the test [6].

Which atmosphere should be used for conditioning?

The governing standard or material specification decides the atmosphere. Both ASTM D618 [14] and ISO 291 [13] list 23 °C and 50 % relative humidity, the former as its standard laboratory atmosphere and the latter among its standard atmospheres.

Is one universal testing machine enough for both tests?

ISO 5893 covers tensile testing systems operating at a constant rate of traverse, along with their use for flexural, shear and compression tests [11]. Whether a given model can do so depends on its force capacity, the grips and flexure fixtures on offer and its strain measurement options, all of which should be confirmed in the supplier's documentation.

Key Takeaways for Plastics Testing Laboratories

Comparable tensile and flexural results for rigid plastics are obtained only when specimen preparation, conditioning, test speed, strain measurement and machine verification are all controlled and recorded. The standards examined here stress this repeatedly [5][6][9]. Regarding these factors as integral to the test, not as background, makes samples, operators and laboratories easier to compare. When buying equipment, start from the standards, specimens and reporting needs, then judge candidate machines against them.

Relevant Testshine Product

Choosing a Universal Testing Machine That Fits Your Tensile and Flexural Testing Needs

Testshine TS-UTM1 Universal Testing Machine

This article has covered the standards, specimens and equipment checks that underlie tensile and flexural testing of rigid plastics. If you are planning such work, the Testshine TS-UTM1 Universal Testing Machine is worth reviewing against the checklist below; its product page publishes its configuration and specifications.

Why it may suit your application, subject to confirmation:

  • A force capacity and force measurement class matched to your strongest specimens and the method you follow.
  • A test speed range spanning the speeds your chosen standards require.
  • Tensile grips, a three point flexure fixture and extensometer or deflection measurement options for your specimens.
  • Calibration and verification documentation for the force measuring system.

Check each point against the published specifications, and ask Testshine to confirm anything not stated for your configuration.

References

  1. International Organization for Standardization, “ISO 527-1:2019, Plastics: Determination of tensile properties, Part 1: General principles,” published July 2019 (catalogue record with scope and life cycle status, Genorma). https://genorma.com/en/standards/iso-527-1-2019/amp

  2. International Organization for Standardization, “ISO 527-2:2025, Plastics: Determination of tensile properties, Part 2: Test conditions for moulding and extrusion plastics,” published June 2025 (catalogue record, Genorma). https://genorma.com/en/standards/iso-527-2-2025

  3. International Organization for Standardization, “ISO 178:2019, Plastics: Determination of flexural properties,” published April 2019 (catalogue record with life cycle status, Genorma). https://genorma.com/en/standards/iso-178-2019

  4. CEN, “EN ISO 178:2019, Plastics: Determination of flexural properties (ISO 178:2019),” 2019 (catalogue record, Genorma). https://genorma.com/en/standards/en-iso-178-2019

  5. ASTM International, “ASTM D638-22, Standard Test Method for Tensile Properties of Plastics,” July 2022. https://store.astm.org/d0638-22.html

  6. ASTM International, “ASTM D638-22, Standard Test Method for Tensile Properties of Plastics,” preview copy, iTeh Standards, 2022. https://cdn.standards.iteh.ai/samples/112891/f899d2918945416cb4ed94b4a005782a/ASTM-D638-22.pdf

  7. ASTM International, “ASTM D790-25, Standard Test Methods for Flexural Properties of Unreinforced and Reinforced Plastics and Electrical Insulating Materials,” 2025. https://store.astm.org/standards/d790

  8. ASTM International, “ASTM D790-25,” scope text, ANSI Webstore, 2025. https://webstore.ansi.org/standards/astm/astmd79025

  9. ASTM International, “ASTM D790-17, Standard Test Methods for Flexural Properties of Unreinforced and Reinforced Plastics and Electrical Insulating Materials,” preview copy, iTeh Standards, 2017 (superseded edition). https://cdn.standards.iteh.ai/samples/97762/3bfa4bc9fbf54c68ad0a721a86682dff/ASTM-D790-17.pdf

  10. International Organization for Standardization, “ISO 20753:2023, Plastics: Test specimens,” November 2023 (AFNOR catalogue record). https://www.boutique.afnor.org/en-gb/standard/iso-207532023/plastics-test-specimens/xs141663/354923

  11. International Organization for Standardization, “ISO 5893:2019, Rubber and plastics test equipment: Tensile, flexural and compression types (constant rate of traverse): Specification,” Edition 4, 2019. https://www.iso.org/standard/77424.html

  12. International Organization for Standardization, “ISO 7500-1:2018, Metallic materials: Calibration and verification of static uniaxial testing machines, Part 1: Tension/compression testing machines,” Edition 5, 2018. https://committee.iso.org/standard/72572.html?browse=ics

  13. International Organization for Standardization, “ISO 291:2008, Plastics: Standard atmospheres for conditioning and testing,” 2008 (iTeh catalogue record). https://standards.iteh.ai/catalog/standards/iso/2789b87b-e33b-4e27-90ed-f0874471893d/iso-291-2008

  14. ASTM International, “ASTM D618-21, Standard Practice for Conditioning Plastics for Testing,” preview copy, iTeh Standards, 2021. https://cdn.standards.iteh.ai/samples/109514/5b390024db1f4d1c9b3cbaa263d1884e/ASTM-D618-21.pdf

  15. Instron, “The Definitive Guide to ISO 178 Flexure Testing for Plastics,” manufacturer technical guide. https://www.instron.com/en/testing-solutions/iso-standards/the-definitive-guide-to-iso-178-flexure-testing-for-plastics

  16. ZwickRoell, “ISO 527-1 and ISO 527-2 Tensile Test on Plastics,” manufacturer technical page. https://www.zwickroell.com/industries/plastics/thermoplastics-and-thermosetting-molding-materials/tensile-test-iso-527-1-2

  17. Intertek, “ISO 527-1 Tensile Testing,” testing laboratory service page. https://www.intertek.com/polymers-plastics/tensile-testing/iso-527-1/

  18. Shimadzu Corporation, “Tensile Test Methods for Plastics: ISO 527 and JIS K 7161, Specs,” manufacturer application page. https://www.shimadzu.com/an/products/materials-testing/uni-ttm-system/tensile-test-methods-for-plastics-iso-527-and-jis-k-7161/spec.html

  19. UL Solutions Prospector, “Flexural Properties, ISO 178,” property reference page. https://plastics.ulprospector.com/properties/ISO178

  20. E. Fernandez, M. Edeleva, L. Cardon and D. R. D’hooge, “Correlating processing induced orientation with tensile properties for mass polymerized acrylonitrile butadiene styrene test specimens,” RSC Applied Polymers, vol. 2, no. 6, pages 1032 to 1042, 2024. DOI: 10.1039/D4LP00238E. https://pubs.rsc.org/en/Content/ArticleLanding/2024/LP/D4LP00238E

  21. International Organization for Standardization, “ISO 5893:2019 table of contents,” as published by DIN. https://www.din.de/de/mitwirken/normenausschuesse/nmp/veroeffentlichungen/wdc-beuth:din21:311945335/toc-3094938/download

  22. International Organization for Standardization, “ISO 20753:2018, Plastics: Test specimens” (withdrawn), 2018. https://www.iso.org/standard/72818.html

  23. Shimadzu Corporation, “Flexural Test Methods for Plastics: ASTM D790,” manufacturer application page. https://www.shimadzu.eu/materials-testing/flexural-test-methods-for-plastics-astm-d790

  24. Estonian Centre for Standardisation and Accreditation, “EVS-EN ISO 527-2:2012, Plastics: Determination of tensile properties, Part 2,” catalogue record (2012 edition, since replaced by ISO 527-2:2025). https://evs.ee/en/evs-en-iso-527-2-2012